Aplicación de Pintura Metálica con Pistola Paso a Paso
Manual paso a paso sobre el ajuste de boquillas, presión de aire y técnica de veladura pulverizada para acabados metálicos homogéneos.
La aplicación de acabados metalizados en oro, plata o pan de oro sobre molduras de poliuretano requiere una técnica de pulverización precisa para evitar manchas y acumulación de partículas metálicas.
Paso 1: Preparación de la Pistola de Gravedad y Boquilla
- Inspect and Clean Polyurethane Substrates — Ensure the rigid polyurethane moulding is completely clean, dry, and free of oil or grease. Lightly abrade the factory-primed surface using grano 180-220 sandpaper to ensure proper paint mechanical keying.
- Execute Joint Cutting and Mounting — Cut moulding ends at precise 45-degree miter angles. Apply polyurethane assembly adhesive to the joint surfaces and backboard; never use silicone. Fasten the profiles mechanically using screws to ensure structural stabilization.
- Seal Fasteners and Apply Secondary Primer — Fill screw heads and miter joint seams with polyurethane-compatible putty. Sand the filled areas smooth with grano 180-220 sandpaper once cured. Apply an optional acrylic or polyurethane primer coat over exposed filler or bare cut edges.
- Prepare Paint and Spray Equipment — Thoroughly mix the solvent-based metallic paint with a mechanical stirrer to suspend all pigments. Pour the paint into a top-gravity feed spray gun fitted with a nozzle size of no greater than 1.3 mm.
- Calibrate Fluid and Air Settings — Adjust the spray gun controls to restrict fluid flow while maintaining high atomizing air pressure. Test the spray fan pattern on a scrap piece to verify fine atomization without wet paint build-up.
- Apply Thin Primary Metallic Coats — Spray two thin, light coats over the polyurethane moulding from a distance of 15–20 cm, using 50% pass overlaps. Periodically shake or stir the top-gravity cup during spraying to prevent metallic pigment settling.
- Execute the Misting (Dusting) Coat — Immediately after the base coat pass, pull the spray gun back to 30–40 cm distance. Apply a light, fast misting pass with low fluid volume to land orientation-controlled metallic flakes uniformly across the surface.
Paso 2: Protocolo de Agitado Continuo de la Mezcla
Los pigmentos metálicos pesados tienden a sedimentar rápidamente en el fondo del depósito; es imprescindible agitar la pistola periódicamente durante la aplicación.
Paso 3: Aplicación en Capas Finas Cruzadas
Ajuste un caudal bajo de pintura con alta presión de aire atomizador. Aplique dos manos muy finas cruzadas sobre la imprimación de fábrica imprimación acrílica blanca monocomponente previamente matizada con lija grano 180-220.
Paso 4: Capa Final de Empolvado y Barniz Protector
Finalice con una pasada rápida de 'empolvado' a mayor distancia para orientar uniformemente las escamas metálicas. Proteja el acabado con barniz acrílico transparente en temperaturas de -100 °C / +80 °C.